Lec 8 - Physics of Welding Arc

Lec 8 - Physics of Welding Arc

Introduction to Joining Technologies for Metals

This section introduces the presentation on joining technologies for metals, specifically focusing on the shielded metal arc welding process and the fundamental principles of arc welding.

Understanding Heat Generation and its Impact on Weld Quality

  • The establishment of a stable arc between the electrode and base metals is crucial for welding.
  • The electrode is connected to the negative terminal and the workpiece to the positive terminal of a power source.
  • Arc initiation methods are used to make the gap between the electrode and workpiece electrically conducting.
  • Two commonly used methods are touch start method (arc initiated by touching electrode to workpiece) and field start method (arc initiated by establishing a high-strength electromagnetic field).
  • Excessive heat generation occurs at contact points during touch start method, leading to partial melting and evaporation.
  • Once the short circuiting is over, creating a gap filled with air, an open circuit voltage or arc voltage is established.
  • Thermal ionization of electrons from electrode tip and ionization of metal vapors occur in this situation.

Flow of Charged Particles in Arc Gap

This section explains how charged particles flow in the arc gap once it becomes electrically conducting.

Touch Start Method vs. Field Start Method

  • In touch start method, electrons move towards cathode (electrode) while ions move towards anode (workpiece).
  • Sufficient charged particle density in the gap makes it electrically conducting, allowing current flow.
  • In field start method, high-strength electromagnetic field helps emission of electrons from cathode without direct contact between electrode and workpiece.

Importance of Gap Conditions for Stable Arc

  • A sufficient potential difference between electrode and workpiece is necessary for a stable arc.
  • Insufficient charged particle density in the gap leads to reduced electrical conductivity and possible arc extinction.
  • High charged particle density ensures good electrical conductivity, resulting in a smooth flow of welding current.

Power of Arc and Heat Generation

This section discusses the power of the arc and its role in generating the desired heat for melting the workpiece.

Initiating the Arc and Generating Heat

  • Two methods are used for initiating the arc: touch start method and field start method.
  • The power of the arc is determined by the product of welding current (flowing through the arc) and arc voltage (potential difference between electrode tip and workpiece).
  • The generated heat from the power of the arc is essential for melting the workpiece during welding.

The transcript does not provide further content beyond this point.

Importance of Good Contact in GTAW Process

This section discusses the importance of good contact between the electrode and the workpiece in the Gas Tungsten Arc Welding (GTAW) process.

  • Poor contact can lead to tungsten inclusion in the weld joints, affecting their soundness.
  • If the tungsten electrode tip is degraded and gets transferred to the weld pool, it can contaminate the weld with tungsten inclusions, negatively impacting mechanical properties.
  • In some cases, direct contact between the electrode and workpiece may not be favorable due to contamination or practical limitations. In such situations, a high-strength electromagnetic field is established to initiate the arc without direct contact.

Initiating Arc Without Direct Contact

This section explains how arc initiation without direct contact is achieved in certain welding processes.

  • In plasma welding and other automatic gas tungsten arc welding processes where direct contact is not suitable or feasible, an arc is initiated without bringing the electrode into contact with the workpiece.
  • This is done by establishing a high-strength electromagnetic field for initiating the arc while feeding the electrode towards the workpiece.

Shielded Metal Arc Welding (SMAW) Process

This section introduces Shielded Metal Arc Welding (SMAW) process and its key components.

  • SMAW uses an electrode coated with flux.
  • The flux coating plays a crucial role in ensuring successful SMAW process.
  • The power source used for SMAW is typically of constant current type, even during short circuit stage.
  • Constant current power source helps maintain consistent heat generation for uniform melting and good quality weld joint.
  • SMAW can use either AC or DC current. DC current is commonly used and compatible with various types of electrodes.

Electrode Selection for SMAW

This section discusses electrode selection for Shielded Metal Arc Welding (SMAW) process.

  • Different types of electrodes, such as rutile, basic, and cellulosic, are commonly used in the industry.
  • DC welding current can be used with all types of electrodes.
  • AC welding requires special care in terms of low ionization potential elements (e.g., sodium, potassium, calcium) present in the electrode to facilitate easy emission of electrons for striking the arc during zero current or voltage changes.

Role of Coating in SMAW Process

This section highlights the role of coating in Shielded Metal Arc Welding (SMAW) process.

  • The top end of the electrode is bare, while the rest is coated with flux.
  • The diameter of the electrode with coating is indicated by "d," and the diameter of the core wire is indicated by "small d."
  • The ratio between core diameter and electrode diameter affects various aspects of SMAW process.

Coating Thickness and Electrode Performance

This section discusses the different values of coating thickness for electrodes and their impact on welding performance.

Coating Thickness and Weld Joint Soundness

  • Thin light coated electrodes have a value ranging from 12 to 135.
  • Medium coated electrodes have a value in the range of 14 to 17.
  • Heavily coated electrodes have a value greater than 17 to 122.
  • The thickness and tenacity of the coating affect the soundness of the weld joint.

Role of Coatings in Electrodes

  • Bare electrodes, such as iron or aluminum, have limited electron emission capability due to higher ionization potential.
  • Coatings with low ionization potential elements (e.g., sodium, potassium, calcium) improve arc stability by providing a conducting gap between the electrode and workpiece.
  • Coatings also help deoxidize metal, separate oxidized metal, and provide flux for removing impurities during welding.

Functions of Coatings in Welding

This section explains additional functions performed by coatings in welding processes.

Controlled Alloying

  • Coatings can incorporate special elements like chromium or molybdenum into the weld pool for controlled alloying.
  • These alloying elements are added in powder form within the coating and transferred to the weld pool during fusion.

Increased Deposition Efficiency

  • Iron powder is incorporated with the coating to increase deposition efficiency.
  • When iron powder melts, it transfers into the weld pool, increasing deposition rate.

Adjusting Viscosity and Surface Tension

  • Coatings can adjust viscosity and surface tension of slag and molten metal during vertical or overhead welding conditions.
  • Thicker and more viscous slag reduces falling tendency of molten metal from the weld pool.

Other Functions of Coatings

  • Coatings can perform functions like adjusting viscosity, surface tension, and reducing flux falling tendency during welding.

The transcript is already in English.

New Section

This section discusses the different elements added to flux in welding and their specific functions.

Elements Added to Flux

  • Quartz is added to increase the current carrying capacity.
  • Magnetite is added for refining the transfer of molten metal drops, achieving split transfer.
  • Calcium carbonate helps reduce arc voltage and provides inactive gases for weld metal protection.
  • Fluorspar increases the viscosity of the slag and molten metal.
  • Ferro manganese and ferro silicon are commonly used as deoxidants.
  • Cellulose releases shielding gases.
  • Potassium water silicate acts as a bonding agent.
  • Rutile, in the form of titanium oxide, increases viscosity and has good arc emission capabilities.

New Section

This section explains the burning of coating material in shielded metal arc welding and its role in protecting weld metal from atmospheric contamination.

Burning of Coating Material

  • The coating material burns out when it approaches the arc during welding.
  • Thermal decomposition and combustion of coating constituents release inactive gases such as CO2 and CO.
  • These gases form a loose cover around the welding arc, protecting the weld metal from atmospheric contamination.

New Section

This section highlights that while shielded metal arc welding provides some protection to weld pool, it forms a loose cover that allows atmospheric gases to interact with reactive metals.

Protection in Shielded Metal Arc Welding

  • Shielded metal arc welding provides a loose cover of CO2 and CO gases around the welding arc.
  • This loose cover may allow atmospheric gases to interact with the weld metal, leading to higher concentrations of oxygen and nitrogen in the weld.
  • Higher concentrations of oxygen and nitrogen can degrade the properties of the weld joint.

New Section

This section explains that shielded metal arc welding is suitable for general-purpose welding but not recommended for reactive metals due to their tendency to react with oxygen.

Limitations of Shielded Metal Arc Welding

  • Shielded metal arc welding is suitable for general-purpose welding and non-critical applications.
  • Reactive metals like aluminum, magnesium, chromium, or stainless steel easily react with oxygen, forming refractory oxide inclusions that interfere with melting and degrade weld quality.
  • More effective protection methods like gas metal arc welding or gas tungsten arc welding are preferred for reactive metals.

New Section

The presentation concludes by summarizing the topics covered: establishing and initiating an arc, conditions necessary for a stable arc, role of different coatings, and electrode selection.

Conclusion

  • The presentation discussed how arcs are established and initiated in welding.
  • It explained the conditions required for striking a stable arc.
  • Different coatings were explored along with their specific functions in flux.
  • Electrode selection was mentioned as an important aspect of shielded metal arc welding.

Turn any video into a summary like this

YouTube links, meetings, lectures. With transcripts, search, and chat.